ORIGINAL ARTICLE
Shear bond strength of dental ceramics to cast commercially pure titanium
Rodrigo GaloI; Deborah Ganga FrizzasI; Renata Cristina Silveira RodriguesII; Ricardo Faria RibeiroIII; Maria da Gloria Chiarello de MattosIII
IDDS, PhD, Post-doctoral student, Department of Prosthodontics and Dental Materials, Ribeirão Preto Dental School, University of São Paulo, Brazil
IIDDS, MS, PhD, Professor, Department of Prosthodontics and Dental Materials, Ribeirão Preto Dental School, University of São Paulo, Brazil
IIIDDS, MS, PhD, Full professor, Department of Prosthodontics and Dental Materials, Ribeirão Preto Dental School, University of São Paulo, Brazil
ABSTRACT
AIM: The objective of this study was to evaluate the bond strength of four dental ceramics to commercially pure titanium.
METHODS: To measure the resistance of metal-ceramic bonding, ceramic rings (Noritake Ti22®, Triceran®, IPS®, Noritake EX-3®) were made around metal rods fused to commercially pure titanium. The area of metal-ceramic union was measured and, after mounting in type III plaster, the rings were subjected to a shearing force in a universal testing machine at a crosshead speed of 2 mm/s until failure occurred. The metal-ceramic shear bond resistance was calculated in MPa.
RESULTS: The shear bond strength means for the ceramics Triceram and Noritake Ti22 (42.50 MPa and 61 MPa, respectively) were higher than the minimum value required by the DIN 13927 standard (25 MPa). The ceramics IPS and Noritake EX3, although not specifically formulated for titanium, also had shear bond strength means above the ISO-recommended value (38.47 MPa and 29.04 MPa, respectively); however, there cracks in some specimens after burning and detachment of the ceramic from the metal.
CONCLUSIONS: The ceramic Noritake Ti22 should be indicated for the commercially pure titanium casting due to its higher mean bond resistance compared to other ceramics utilized.
Keywords: shear bond strength, titanium ceramic system, low firing ceramic.
Full text available only in PDF format.
References
1.Atsü S, Berksun S. Bond strength of three porcelains to two forms of titanium using two firing atmospheres. J Prosthet Dent. 2000; 84: 567-74. [ Links ]
2.Cai Z, Bunce N, Nunn ME, Okabe T. Porcelain adherence to dental cast CP titanium: effects of surface modifications. Biomaterials. 2001; 22: 979-86. [ Links ]
3.Oshida Y, Reyes MJ. Titanium-porcelain system. Part IV: some mechanistic considerations on porcelain bond strengths. Biomed Mater Eng. 2001; 11: 137-42. [ Links ]
4.Könönen M, Kivilahti J. Fusing of dental ceramics to titanium. J Dent Res. 2001; 80: 848-54. [ Links ]
5.Hautaniemi JA, Hero H, Juhanoja JT. On the bonding of porcelain on titanium. J Mater Sci. 1992; 3: 186-91. [ Links ]
6.Wang RR, Fenton A. Titanium for prosthodontics applications: A review of the literature. Quintessence Int. 1996; 27: 401-8. [ Links ]
7.Kimura H, Hong CJ, Okazaki M, Takahashi J. Oxidation effects on porcelain-titanium interface reactions and bond strength. Dent Mater J. 1990; 9: 91-9. [ Links ]
8.Al Hussaini I, Al Wazzan KA. Effect of surface treatment on bond strength of low-fusing porcelain to commercially pure titanium. J Prosthet Dent. 2005; 94: 350-6. [ Links ]
9.Ida K, Togaya T, Tsutsumi S, Suzuki M. Mechanical properties of pure titanium and titanium alloys- evaluation for dental casting metals. J Jpn Dent Mater. 1983; 2: 765-71. [ Links ]
10.Yilmaz H, Dincer C. Comparison of the bond compatibility of titanium and an Ni-Cr alloy to dental porcelain. J Dent. 1999; 27: 215-22. [ Links ]
11.Hanawa T, Kon M, Ohkawa S, Asaoka K. Diffusion of elements in porcelain into titanium oxide. Dent Mater J. 1994; 13: 164-73. [ Links ]
12.Tarozzo LSA, de Mattos MDC, Ribeiro RF, Semprini M. Comparison of retentive systems for composites used as alternatives to porcelain in fixed partial dentures. J Prosthet Dent. 2003; 89: 572-8. [ Links ]
13.Galo R, Ribeiro RF, Rodrigues RC, Pagnano VO, Mattos MG. Effect of laser welding on the titanium composite tensile bond strength. Braz Dent J. 2009; 20: 403-9. [ Links ]
14.German Standard Institution. DIN 13927 Metal-Ceramic System. Berlin: Beuth Verlag; 1990. [ Links ]
15.White SN, Ho L, AA Caputo, Goo E. Strength of porcelain fused to titanium beams. J Prosthet Dent. 1996; 75: 640-8. [ Links ]
16.Adachi M, Mackert J, Parry E, Fairhurst C. Oxide adherence and porcelain bonding to titanium and Ti6Al4V alloy. J Dent Res. 1990; 6: 1230-5. [ Links ]
17.Pröbster L, Maiwald U, Weber H. Three-point bending strength of ceramics fused to cast titanium. Eur J Oral Sci. 1996; 104: 313-9. [ Links ]
18.Derand T, Herø H. Bond strength of porcelain on cast vs wrought titanium. Scand J Dent Res. 1992; 100: 184-8. [ Links ]
19.Lenz J, Schwarz S, Schwickerath H, Sperner F, Schäfer A. Bond strength of metalceramic systems in three-point flexural bond test. J Appl Biomater. 1995; 6: 55-64. [ Links ]
20.Könönen M, Kivilathi J. Bonding of low-fusing dental porcelain to commercially pure titanium. J Biomed Res. 1994; 28: 1027-35. [ Links ]
21.Yoda M, Konno T, Takada Y, Iijima K, Griggs J, Okuno O. Bond strength of binary titanium alloys to porcelain. Biomaterials. 2001; 22: 1675-81. [ Links ]
22.Troia M, Henriques G, Nobilo M, Mesquita M. The effect of thermal cycling on the bond strength of low-fusing porcelain to commercially pure titanium and titaniumaluminumvanadium alloy. Dent Mater. 2003; 19: 790-6. [ Links ]
Correspondence to:
Maria da Gloria Chiarello de Mattos
Department of Prosthodontics and Dental Materials
FORP/USP. Av. do Café s/n, Monte Alegre, 14040-904 Ribeirão Preto, Brasil
Phone: +55 16 3602-4098
Fax : +55 16 3602-4780
E-mail: gloria@forp.usp.br
Received for publication: March 16, 2010
Accepted: August 02, 2010